Amine stress corrosion cracking (ASCC) is a costly problem that can damage critical equipment, causing unplanned shutdowns, environmental issues, and financial losses. It occurs when corrosive amine environments, changing temperatures, and mechanical stresses combine—often in key parts of amine regeneration units. Understanding how ASCC develops is the first step toward effective prevention.
This comprehensive guide explores the causes, effects, and most importantly, the solutions to amine stress corrosion cracking. Drawing on decades of industry experience and research, we’ll examine how modern protection technologies are revolutionizing amine corrosion management and extending the operational life of these mission-critical assets.
Amine stress corrosion cracking (ASCC) is a form of alkaline stress corrosion cracking specifically targeting carbon and low alloy steels in lean amine environments. It’s important to note that this is distinct from the cracking in rich amine systems, which is actually a form of wet H₂S cracking (also known as sulfide stress cracking). ASCC is common in amine regeneration units where the combination of corrosive chemicals, high temperatures, and mechanical stress creates ideal conditions for this type of corrosion.
ASCC primarily affects facilities in:
- Oil and gas production
- Refineries
- Natural gas processing
- Petrochemical manufacturing
- Carbon capture systems
The Amine Regeneration Process and Corrosion Risk
The amine regeneration process is fundamental to gas sweetening operations, removing acid gases (H₂S and CO₂) from hydrocarbon streams. This critical process involves several key components:
- Amine absorber/contactor – where sour gas contacts the amine solution
- Amine flash tank – where hydrocarbon vapors are removed
- Amine regenerator column – where acid gases are stripped from the rich amine
- Amine reboiler – where heat is applied to facilitate regeneration
According to industry data, almost 50% of corrosion in amine systems occurs in the hottest parts of the plant – the amine reboiler and the bottom of the amine regenerator column. This is mainly because corrosion rates accelerate at higher temperatures, with acid gas breakout creating highly corrosive conditions.
Mechanisms & Causes of Amine Stress Corrosion Cracking
Amine unit corrosion in refineries occurs through several interrelated mechanisms that can be categorized into chemical, operational, and metallurgical factors.
Chemical Factors
Amine type and concentration play a significant role in corrosion susceptibility, as different amines (MEA, DEA, MDEA, DGA) exhibit varying corrosivity profiles based on their chemical structure and reactivity. A comprehensive NACE survey of 294 amine units (272 refineries) found 164 reported stress corrosion cracking cases in MEA systems, compared to just 37 in DEA and 30 in other amines like ADIP. The study revealed that cracking was predominantly intergranular and oxide-filled, occurring most frequently in weld heat-affected zones (HAZs).
H₂S and CO₂ levels strongly affect corrosion risk—higher acid gas loading makes conditions more aggressive. Heat-stable salts formed from contaminants reduce amine effectiveness and increase corrosivity. Oxygen ingress accelerates corrosion by oxidizing sulfides and creating new corrosive species. Even small pH shifts can significantly change corrosion rates and cracking risk.
Operational Factors
Temperature is perhaps the most significant factor in operational influences, as elevated temperatures in the amine regeneration unit accelerate corrosion reactions exponentially. Pressure fluctuations during operation create stress cycles that can initiate and propagate cracks in susceptible materials. Two-phase flow conditions, where liquid and gas phases coexist, cause erosion-corrosion in piping and vessels due to the impingement of droplets on metal surfaces. Flashing conditions, where pressure drops cause rapid vaporization, lead to localized attack and pitting as corrosive species concentrate at the metal surface. Velocity effects are also crucial, as high-velocity areas experience flow-enhanced corrosion due to increased mass transfer rates and potential protective film damage.
Explore IGS capabilities
Discover how IGS helps operators improve asset performance through engineered solutions for asset integrity, life extension and energy efficiency.
Materials Affected by Amine Stress Corrosion Cracking
Carbon Steel:
Due to cost considerations, most amine vessels and piping are constructed from carbon steel. While generally acceptable for amine service, carbon steel is susceptible to general corrosion, pitting, and stress corrosion cracking, particularly in hot, regenerated amine service.
Stainless Steels:
Austenitic stainless steels (304, 316) offer improved resistance to amine plant corrosion but can still suffer from chloride-induced stress corrosion cracking, particularly at weld heat-affected zones.
High-Alloy Materials:
Alloys with higher nickel and molybdenum content (e.g., Inconel, Hastelloy) provide excellent resistance but at significantly higher cost, making them suitable only for critical components in severe service.
Prevention & Mitigation Strategies for Amine Corrosion
There are effective amine corrosion management methods available that require a multi-faceted approach.
Material Selection
- Use appropriate corrosion allowances based on expected service life
- Consider composite construction with CRA cladding in critical areas
- Specify post-weld heat treatment to reduce residual stresses
- Implement proper weld procedures to minimize susceptible microstructures
Process Control
- Maintain recommended amine concentration and loading limits
- Control solution temperature, especially in the reboiler
- Implement effective filtration to remove suspended solids
- Regular analysis and maintenance of amine chemistry
- Monitor and control oxygen ingress
Advanced Amine Corrosion Control Technologies
Modern corrosion prevention strategies include innovative approaches like HVTS® (High Velocity Thermal Spray) cladding systems. Unlike traditional methods, HVTS® offers several advantages:
- Application without heat-affected zones
- 3× faster application than welding
- Compatible with existing weld overlays
- Superior corrosion/erosion resistance
- No need for post-weld heat treatment
- Superior mechanical properties compared to organic coatings
- Wide service temperature and pressure ranges
- Ability to be applied in-situ during scheduled turnarounds
- Long-term protection against all forms of sweet corrosion and sour gas attack
Industry Adoption of HVTS® Technology for Amine System Protection
HVTS® technology has become increasingly recognized as a standard practice for protecting amine systems across the oil and gas industry. Major energy companies including Phillips 66, Shell, ExxonMobil, Chevron, and BP have adopted this technology as their preferred solution for amine unit corrosion protection. The widespread implementation of HVTS® in facilities across North America, Europe, and the Middle East demonstrates its effectiveness and reliability in combating amine stress corrosion cracking.
Case Study
Midstream Amine Still Corrosion Solution
During a scheduled turnaround inspection, a Phillips 66 gas treating facility in Giddings, TX discovered severe corrosion damage in the main amine regenerator column between trays 13 and 18. The damage was directly attributed to aggressive amine attack on the carbon steel shell.

Previous Mitigation Attempts
The facility had historically relied on reactive approaches:
- Periodic weld buildup to maintain minimum thickness requirements
- Application of organic coatings on a 5-year turnaround cycle
These methods proved ineffective and costly, as the organic coatings failed prematurely, and required recurring repairs.
HVTS® Solution Implementation
After exploring several coating options that failed to provide guaranteed protection against amine exposure and high temperatures, Phillips 66 consulted with their refining division. IGS HVTS® (High Velocity Thermal Spray) technology was selected as the permanent solution based on excellent performance in amine units across multiple refineries.
The HVTS® application covered 277 square feet of the vessel interior and was completed in just 5 shifts. Critically, the process introduced no heat-affected zones and required no post-weld heat treatment, significantly reducing downtime compared to traditional weld overlay methods.
Results and Long-Term Benefits
By implementing the HVTS® cladding system, Phillips 66 effectively:
- Eliminated the need for recurring repairs in this problem area
- Reduced the total cost of ownership for the asset
- Created a permanent barrier against amine stress corrosion cracking
- Minimized future maintenance requirements and associated downtime
The facility scheduled the next inspection for its next shutdown in five years. During this inspection, thickness readings will be compared against the original application map to verify cladding integrity and performance.
Additional Implementation Examples
Beyond Phillips 66, numerous other facilities have successfully implemented HVTS® technology to address amine corrosion challenges.
- Shell has standardized HVTS® applications in their amine regeneration units across multiple refineries, reporting significant maintenance costs and extended equipment life reductions.
- ExxonMobil facilities have utilized HVTS® cladding for MDEA units, effectively eliminating recurring corrosion issues in previously problematic areas.
- Chevron has implemented HVTS® solutions in both refinery and gas processing amine units, establishing it as their preferred method for addressing stress corrosion cracking in these critical systems.
- Several Middle Eastern national oil companies have adopted HVTS® technology as their standard specification for new amine units and retrofits, based on proven performance in harsh operating environments.
- European refiners have increasingly turned to HVTS® as a permanent solution for amine reboilers and regenerator columns, reporting substantial improvements in equipment reliability and reduced maintenance costs.
Conclusion
Amine stress corrosion cracking is a significant challenge in oil and gas processing operations. Operators can effectively manage internal pipeline and amine plant corrosion by correctly understanding the underlying mechanisms, implementing appropriate materials, and applying advanced protection systems like HVTS® cladding.
A proactive approach to amine corrosion control will ensure reliable operation, extend asset life, and avoid the substantial costs associated with corrosion-related failures. Investment in proper corrosion mitigation strategies pays dividends through improved safety, reduced downtime, and enhanced operational efficiency.
For more information on advanced solutions for pipeline corrosion prevention, contact our corrosion specialists today.
Book a Free Technical Evaluation
More corrosion and erosion management articles from Integrated Global Services:
CO₂ Corrosion Prevention and Control in Oil and Gas Production
Preventing Wet CO₂ Corrosion in Carbon Capture and Storage Project
How to Prevent Microbially Influenced Corrosion (MIC) with On-Site Alloy Upgrade
Why is High Emissivity Coating Durability Important in Fired Heaters?
Strategies for Preventing Internal Pipeline Corrosion in the Energy Industry
Flue Gas Dew Point Corrosion Mitigation: Alloy Upgrading Techniques
Mitigating Metal Dusting Corrosion in Ammonia and Methanol Reformers
Combating Flow Accelerated Corrosion in Power Plants with IGS HVTS Technology
Why an Alloy Upgrade is the Best Solution to Crude Unit Overhead Corrosion Control
Protecting Hydropower Turbines from Corrosion with HVTS Coatings
Protecting Offshore Wind Turbines – Splash Zone Corrosion
The Critical Role of High Emissivity Coatings in Space Exploration
Organic Coatings in Pressure Vessels: Internal Coating Failure Analysis
How to Stop Corrosion on Your Refinery Distillation Column
Causes of Boiler Corrosion and Benefits of Boiler Tube Coating
5 Common Causes of Refractory Failure and How to Fix Them
Boiler Tube Leaks Prevented with Proactive Maintenance
Understanding Oil & Gas CO2 and NOx Emissions, and the Science Behind Reducing Them